Copper-Tin-Lead-Alloys

Sprache / Language / Langue

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 491 K

83,0 – 87,0

< 0,01

< 0,3

< 2,0

< 0,10

4,0 – 6,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn5Zn5Pb5-C

< 0,25

< 0,01

4,0 – 6,0

4,0 – 6,0

       

Comments:
Construction material, easy to cast, can be soldered in
a soft condition and with limited hardness, sea-water-resistant

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

250

110

13

65

Continuous casting GC

250

110

13

65

Notes for Use: Water and steam fittings up to 225°C, pump parts subjected to normal stresses

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 493 K

81,0 – 85,0

< 0,01

< 0,2

< 2,0

< 0,10

5,0 – 8,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn7Zn4Pb7-C

< 0,3

< 0,01

6,0 – 8,0

2,0 – 5,0

       

Comments:
Medium-hard sliding-bearing material with good emergency-running characteristics

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

260

120

12

70

Continuous casting GC

260

120

12

70

Notes for Use: Axle-bearing and sliding-bearing shells for general mechanical engeneering (peak loads of p up to 4000 N/cm2 permissible), sliding rails subjected to medium stresses, sliding-bearing bushes subjected to normal und high stresses, neck bushes and stuffing boxes lining, cylinder insert brushes

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 494 K

80,0 – 87,0

< 0,01

< 0,25 < 0,2

< 2,0

< 0,10

8,0 – 10,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn5Zn4Pb9-C

< 0,5

< 0,01

4,0 – 6,0

< 2,0

       

Comments:
Sliding material, „soft“ material

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

200

90

6

60

Continuous casting GC

200

100

9

60

Notes for Use: Bearing bushes, sliding bearings

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 495 K

78,0 – 82,0

< 0,01

< 0,25 < 0,2

< 2,0

< 0,10

8,0 – 11,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn10Pb10-C

< 0,5

< 0,01

9,0 – 11,0

< 2,0

       

Comments:
 Bearing material with good sliding characteristics and a good wear resistance, good corrosion resistance

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

220

110

6

70

Continuous casting GC

220

110

8

70

Notes for Use: Sliding bearings with high surface pressures where edge-pressure phenomena may occur, peak stressing in the case of good lubrication: up to p = 6000 N/cm²

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 496 K

74,0 – 80,0

< 0,01

< 0,25 < 0,2

0,5 – 2,0

< 0,10

13,0 – 17,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn7Pb15-C

< 0,5

< 0,01

6,0 – 8,0

< 2,0

       

Comments:
Bearing material with good sliding and emergency-running characteristics in the case of tempory lack of lubricant and in the case of water lubrication, resistant to sulphuric acid

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

200

90

7

65

Continuous casting GC

200

90

8

65

Notes for Use: Bearings with high surface pressures where edge-pressure phenomena may occur, peak stressing in the case of good lubrication: up to p = 5000 N/cm²

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Fe

Mn

Ni

P

Pb

S

CC 497 K

70,0 – 78,0

< 0,01

< 0,25 < 0,2

0,5 – 2,5

< 0,10

18,0 – 23,0

< 0,1

Code

Sb

Si

Sn

Zn

       

CuSn5Pb20-C

< 0,75

< 0,01

4,0 – 6,0

< 2,0

       

Comments:
Bearing material with the best sliding characteristics, particular good emergency-running characteristics in the case ofa tempory lack of lubricant and in the case of water lubrication

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

170

80

6

50

Continuous casting GC

180

90

8

50

Notes for Use: Bearings also with high sliding speeds, peak stressing in the case of good lubrication up to p = 4000 N/cm²