Copper-Aluminium-Alloys

Sprache / Language / Langue

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Bi

Cr

Fe

Mg

Mn

Ni

CC 331 G

83,0 – 89,5

8,5 – 10,5

1,5 – 3,5

< 0,05

< 1,0

< 1,5

Code

Pb

Si

Sn

Zn

       

CuAl10Fe2-C

< 0,10

< 0,2

< 0,2

< 0,5

       

Comments:
Construction material, only slight temperature dependence between –200°C and +200°C

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

550

200

18

130

Continuous casting GC

550

200

15

130

Notes for Use: Parts subjected to mechanical stresses: bushes, pinions and bevel gears, syncronous rings, in textile machines and automobile construction

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Bi

Cr

Fe

Mg

Mn

Ni

CC 333 G

76,0 – 83,0

8,5 – 10,5

< 0,01

< 0,05

4,0 – 5,5

< 0,05

< 3,0

4,0 – 6,0

Code

Pb

Si

Sn

Zn

       

CuAl10Fe5Ni5-C

< 0,03

< 0,1

< 0,1

< 0,5

       

Comments:
Construction material with a further improvement in the strength characteristics, resistant in cold and hot sea-water, good fatigue endurance limit

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

650

280

13

150

Continuous casting GC

650

280

13

150

Notes for Use: Parts subjected to high stresses with regard to strength and corrosion resistance, superheated-steam fittings and manifolds in apparatus, engeneering and in the petrochemical industry, sliding bearings with very high impact loads, worm gears and helical gears, articulated jaws and forcing nuts

 

Code Designation According to
DIN EN 1982

Composition of the Alloys in Percent (Proportions by Mass)

Number

Cu

Al

Bi

Cr

Fe

Mg

Mn

Ni

CC 334 G

72,0 – 78,0

10,0 – 12,0

4,0 – 7,0

< 0,05

< 2,5

4,0 – 7,5

Code

Pb

Si

Sn

Zn

       

CuAl11Fe6Ni6-C

< 0,05

< 0,1

< 0,2

< 0,5

       

Comments:
Construction material with high strength characteristics, resistant in cold and hot sea-water, very good fatigue endurance limit, very cavitation-resistant, high load capacity with a good wear resistance, good lubrication necessary

Casting Process and Designation

Mechanical Characteristics

Tensile Strength
Rm N/mm 2 min.

0,2 % Offset Yield Strength
0,2 % Rp 0,2 N/mm 2 min.

Elongation at Fracture
% A % min.

Brinell Hardness
HB min.

Centrifugal casting GZ

750

380

5

185

Continuous casting GC

750

380

3

190

Notes for Use: Like CC 333 G, but more stringent requirements on the cavitation resistance and/or wear resistance